WORKSHOP RECIPES AND FORMULAS
In a work of this kind, dealing with
the various elements, the boy should have at hand
recipes or formulas for everything which comes within
the province of his experiments. The following
are most carefully selected, the objects being to
present those which are the more easily compounded.
ADHESIVES FOR VARIOUS USES.-Waterproof
glue. Use a good quality of glue, and dissolve
it in warm water, then add one pound of linseed oil
to eight pounds of the glue. Add three ounces
of nitric acid.
Leather or Card-board Glue. After
dissolving good glue in water, to which a little turpentine
has been added, mix it with a thick paste of starch,
the proportion of starch to glue being about two to
every part of glue used. The mixture is used
cold.
A fine Belt Glue. Dissolve 50
ounces of gelatine in water, and heat after pouring
off the excess water. Then stir in five ounces
of glycerine, ten ounces of turpentine, and five ounces
of linseed oil varnish. If too thick add water
to suit.
For cementing Iron to Marble.
Use 30 parts of Plaster of Paris, 10 parts of iron
filings, and one half part of sal ammoniac.
These are mixed up with vinegar to make a fluid paste.
To cement Glass to Iron. Use
3 ounces of boiled linseed oil and 1 part of copal
varnish, and into this put 2 ounces of litharge and
1 ounce of white lead and thoroughly mingle so as
to make a smooth paste.
Water-proof Cement. Boiled linseed
oil, 6 ounces; copal, 6 ounces; litharge, 2 ounces;
and white lead, 16 ounces. To be thoroughly incorporated.
To unite rubber or leather to hard
substances. One ounce of pulverized gum shellac
dissolved in 9-1/2 ounces of strong ammonia, will make
an elastic cement. Must be kept tightly corked.
For uniting iron to iron. Use
equal parts of boiled oil, white lead, pipe clay and
black oxide of manganese, and form it into a paste.
Transparent Cement. Unite 1 ounce
of india rubber, 67 ounces of chloroform, and 40 ounces
of mastic. This is to be kept together for a
week, and stirred at times, when it will be ready for
use.
To Attach Cloth to Metal. Water
100 parts, sugar 10 parts, starch 20 parts, and zinc
chloride 1 part. This must be first stirred and
made free of lumps, and then heated until it thickens.
United States Government Gum.
Dissolve 1 part of gum arabic in water and add 4 parts
of sugar and 1 part of starch. This is then boiled
for a few minutes, and thinned down as required.
TO MAKE DIFFERENT ALLOYS.-Silver-aluminum.
Silver one-fourth part, and aluminum three-fourth
parts.
Bell-metal. Copper, 80 parts;
tin, 20 parts. Or, copper, 72 parts; tin, 26
parts; zinc, 2 parts. Or, copper 2; 1 of tin.
Brass. Copper, 66 parts; zinc,
32 parts; tin, 1 part; lead, 1 part.
Bronzes. Copper, 65 parts; zinc,
30 parts; tin, 5 parts. Or, copper, 85 parts;
zinc, 10 parts; tin, 3 parts; lead, 2 parts.
German Silve parts of copper;
26 parts zinc; 22 parts nickel.
For Coating Mirrors. Tin, 70 parts; mercury,
30 parts.
BOILER COMPOUNDS.-To prevent scaling.
Use common washing soda, or
Glauber salts.
TO DISSOLVE CELLULOID.-Use
50 parts of alcohol and 5 parts of camphor for every
5 parts of celluloid. When the celluloid is put
into the solution it will dissolve it.
To Soften Celluloid. This may
be done by simply heating, so it will bend, and by
putting it in steam, it can be worked like dough.
CLAY MIXTURE FOR FORGES.-Mix
dry 20 parts of fire clay, 20 parts cast-iron turnings,
one part of common salt, and 1/2 part sal ammoniac,
and then add water while stirring, so as to form a
mortar of the proper consistency. The mixture
will become very hard when heat is applied.
A Modeling Clay. This is made
by mixing the clay with glycerine and afterwards adding
vaseline. If too much vaseline is added
it becomes too soft.
FLUIDS FOR CLEANING CLOTHES, FURNITURE,
ETC.-For Delicate Fabrics. Make strong
decoction of soap bark, and put into alcohol.
Non-inflammable Cleaner. Equal
parts of acetone, ammonia and diluted alcohol.
Taking dried paint from clothing.
Shake up 2 parts of ammonia water with 1 part of spirits
of turpentine.
Cleaning Furniture, etc.
Unite 2.4 parts of wax; 9.4 parts of oil of turpentine;
42 parts acetic acid; 42 parts citric acid; 42 parts
white soap. This must be well mingled before
using.
Removing Rust from Iron or Steel.
Rub the surface with oil of tartar. Or, apply
turpentine or kerosene, and after allowing to stand
over night, clean with emery cloth.
For Removing Ink Stains from Silver.
Use a paste made of chloride of lime and water.
To clean Silver-Plated Ware.
Make a mixture of cream of tartar, 2 parts; levigated
chalk, 2 parts; and alum, 1 part. Grind up the
alum and mix thoroughly.
Cleaning a Gas Stove. Make a
solution of 9 parts of caustic soda and 150 parts
of water, and put the separate parts of the stove in
the solution for an hour or two. The parts will
come out looking like new.
Cleaning Aluminum. A few drops
of sulphuric acid in water will restore the luster
to aluminum ware.
Oil Eradicator. Soap spirits,
100 parts; ammonia solution, 25; acetic ether, 15
parts.
DISINFECTANTS.-Camphor,
1 ounce; carbolic acid (75 per cent.), 12 ounces;
aqua ammonia, 10 drachms; soft salt water, 8 drachms.
Water-Closet Deodorant. Ferric
chloride, 4 parts; zinc chloride, 5 parts; aluminum
chloride, 4 parts; calcium chloride, 5 parts; magnesium
chloride, 3 parts; and water sufficient to make 90
parts. When all is dissolved add to each gallon
10 grains of thymol and a quarter-ounce of rosemary
that had been previously dissolved in six quarts of
alcohol.
Odorless Disinfectants. Mercuric
chloride, 1 part; cupric sulphate, 10 parts; zinc
sulphate, 50 parts; sodium chloride, 65 parts; water
to make 1,000 parts.
Emery for Lapping Purposes. Fill
a pint bottle with machine oil and emery flour, in
the proportion of 7 parts oil and 1 part emery.
Allow it to stand for twenty minutes, after shaking
up well, then pour off half the contents, without
disturbing the settlings, and the part so poured off
contains only the finest of the emery particles, and
is the only part which should be used on the lapping
roller.
EXPLOSIVES.-Common Gunpowder.
Potassium nitrate, 75 parts; charcoal, 15 parts; sulphur,
10 parts.
Dynamit per cent. nitro-glycerine;
25 per cent. infusorial earth.
Giant Powde per cent. nitro-glycerine;
48 per cent. nitrate of potash; 8 per cent. of sulphur;
8 per cent. charcoal.
Fulminate. Chlorate of potassia,
6 parts; pure lampblack, 4 parts; sulphur, 1 part.
A blow will cause it to explode.
FILES.-How to Keep Clean.
Olive oil is the proper substance to rub over files,
as this will prevent the creases from filling up while
in use, and preserve the file for a longer time, and
also enable it to do better cutting.
To Renew Old Files. Use a potash
bath for boiling them in, and afterwards brush them
well so as to get the creases clean. Then stretch
a cotton cloth between two supports, and after plunging
the file into nitric acid, use the stretched cloth
to wipe off the acid. The object is to remove
the acid from the ridges of the file, so the acid will
only eat out or etch the deep portions between the
ridges, and not affect the edges or teeth.
FIRE PROOF MATERIALS OR SUBSTANCES.-For
Wood. For the kind where it is desired to apply
with a brush, use 100 parts sodium silicate; 50 parts
of Spanish white, and 100 parts of glue. It must
be applied hot.
Another good preparation is made as
follows: Sodium silicate, 350 parts; asbestos,
powdered, 350 parts; and boiling water 1,000 parts.
For Coating Steel, etc.
Silica, 50 parts; plastic fire clay, 10 parts; ball
clay, 3 parts. To be thoroughly mixed.
For Paper. Ammonium sulphate,
8 parts; boracic acid, 3 parts; borax, 2 parts; water,
100 parts. This is applied in a liquid state to
the paper surface.
FLOOR DRESSINGS.-Oil Stain.
Neats’ foot oil, 1 part; cottonseed oil, 1 part;
petroleum oil, 1 part. This may be colored with
anything desired, like burnt sienna, annatto, or other
coloring material.
Ballroom Powder. Hard paraffine,
1 pound; powdered boric acid, 7 pounds; oil of lavender,
1 drachm; oil of neroli, 20 minims.
FOOT POWDERS.-For Perspiring
Feet. Balsam Peru, 15 minims; formic acid, 1
drachm; chloral hydrate, 1 drachm; alcohol to make
3 ounces.
For Easing Feet. Tannaform, 1
drachm; talcum, 2 drachms; lycopodium, 30 grains.
Frost Bites. Carbolized water,
4 drachms; nitric acid, 1 drop; oil of geranium, 1
drop.
GLASS.-To cut glass, hold
it under water, and use a pair of shears.
To make a hole through glass, place
a circle of moist earth on the glass, and form a hole
in this the diameter wanted for the hole, and in this
hole pour molten lead, and the part touched by the
lead will fall out.
To Frost Glass. Cover it with
a mixture of 6 ounces of magnesium sulphate, 2 ounces
of dextrine, and 20 ounces of water. This produces
a fine effect.
To imitate ground glass, use a composition
of sandarac, 2-1/2 ounces; mastic, 1/2 ounce; ether,
24 ounces; and benzine, 16 ounces.
IRON AND STEEL.-How to
distinguish them. Wash the metal and put it into
a solution of bichromate of potash to which has been
added a small amount of sulphuric acid. In a
minute or so take out the metal, wash and wipe it.
Soft steel and cast iron will have the appearance of
an ash-gray tint; tempered steels will be black; and
puddled or refined irons will be nearly white and
have a metallic reflection.
To Harden Iron or Steel. If wrought
iron, put in the charge 20 parts, by weight, of common
salt, 2 parts of potassium cyanide, .3 part of potassium
bichromate, .15 part of broken glass.
To harden cast iron, there should
be added to the charge the following: To 60 parts
of water, add 2-1/2 parts of vinegar, 3 parts of common
salt, and .25 part of hydrochloric acid.
To soften castings: Heat them
to a high temperature and cover them with fine coal
dust and allow to cool gradually.
LACQUERS.-For Aluminum.
Dissolve 100 parts of gum lac in 300 parts of
ammonia and heat for an hour moderately in a water
bath. The aluminum must be well cleaned before
applying. Heat the aluminum plate afterwards.
For Brass. Make a compound as
follows; Annatto, 1/4 ounce; saffro, 1/4 ounce; turmeric,
1 ounce; seed lac, 3 ounces; and alcohol, 1 pint.
Allow the mixture to stand for three days, then strain
in the vessel which contains the seed lac, and
allow to stand until all is dissolved.
For Copper. Heat fine, thickly
liquid amber varnish so it can be readily applied
to the copper, and this is allowed to dry. Then
heat the coated object until it commences to smoke
and turn brown.
LUBRICANTS.-Heavy machinery
oils. Use paraffine, 8 pounds; palm
oil, 20 pounds; and oleonaptha, 12 pounds. Dissolve
the paraffine in the oleonaptha at a temperature
of 160 degrees and then stir in the palm oil a little
at a time.
For Cutting Tools. Heat six gallons
of water and put in three and a half pounds of soft
soap and a half gallon of clean refuse oil. It
should be well mixed.
For high-speed bearings. Use
flaky graphite and kerosene oil. Apply this as
soon as there is any indication of heating in the bearings.
For lathe centers, one part of graphite
and four parts of tallow thoroughly mixed and applied
will be very serviceable.
For Wooden Gears. Use tallow,
30 parts; palm oil; 20 parts; fish oil, 10 parts;
and graphite, 20 parts.
PAPER.-FIRE PROOF PAPER.-Make
the following solution: Ammonium sulphate, 8
parts; boracic acid, 3 parts; water, 100 parts.
Mix at a temperature of 120 degrees. Paper coated
with this will resist heat.
Filter Paper. Dip the paper into
nitric acid of 1.433 specific gravity, and subsequently
wash and dry it. This makes a fine filtering body.
Carbon Paper. A variety of substances
may be used, such as fine soot or ivory black, ultramarine
or Paris blue. Mix either with fine grain soap,
so it is of a uniform consistency and then apply to
the paper with a stiff brush, rubbing it in until
it is evenly spread over the surface.
Tracing Paper. Take unsized paper
and apply a coat of varnish made of equal parts of
Canada balsam and oil of turpentine. To increase
the transparency give another coat. The sheets
must be well dried before using.
PHOTOGRAPHY.-Developers.
1. Pure water, 30 ounces; sulphite
soda, 5 ounces; carbonate soda, 2-1/2 ounces.
2. Pure water, 24 ounces; oxalic
acid, 15 grains; pyrogallic acid, 1 ounce.
To develop use of solution 1, 1 ounce;
solution 2, 1/2 ounce; and water, 3 ounces.
Stock solutions for developing:
Make solution N as follows: water, 32 ounces;
tolidol, I ounce; sodium sulphate, 1-1/2 ounces.
Solution N: Water, 32 ounces; sodium sulphate.
Solution N: Water, 32 ounces; sodium carbonate,
from 4 to 6 ounces.
Fixing bath. Add two ounces of
S. P. C. clarifier (acid bisulphate of sodium) solution
to one quart of hypo solution 1 in 5.
Clearing solution. Saturated
solution of alum, 20 ounces; and hydrochloric acid,
1 ounce. Varnish. Brush over the negative
a solution of equal parts of benzol and Japanese gold
size.
PLASTERS.-Court Plaster.
Use good quality silk, and on this spread a solution
of isinglass warmed. Dry and repeat several times,
then apply several coats of balsam of Peru. Or,
On muslin or silk properly stretched,
apply a thin coating of smooth strained flour paste,
and when dry several coats of colorless gelatine are
added. The gelatine is applied warm, and cooled
before the fabric is taken off.
PLATING.-Bronze coating.
For antiques, use vinegar, 1,000 parts; by weight,
powdered bloodstone, 125 parts; plumbago, 25 parts.
Apply with brush.
For brass where a copper surface is
desired, make a rouge with a little chloride of platinum
and water, and apply with a brush.
For gas fixtures. Use a bronze
paint and mix with it five times its volume of spirit
of turpentine, and to this mixture add dried slaked
lime, about 40 grains to the pint. Agitate well
and decant the clear liquid.
COLORING METALS.-Brilliant
black for iron. Selenious acid, 6 parts; cupric
sulphate, 10 parts; water 1,000 parts; nitric acid,
5 parts.
Blue-black. Selenious acid, 10
parts; nitric acid, 5 parts; cupric sulphate; water,
1,000 parts. The colors will be varied dependent
on the time the objects are immersed in the solution.
Brass may be colored brown by using
an acid solution of nitrate of silver and bismuth;
or a light bronze by an acid solution of nitrate of
silver and copper; or black by a solution of nitrate
of copper.
To copper plate aluminum, take 30
parts of sulphate of copper; 30 parts of cream of
tartar; 25 parts of soda; and 1,000 parts of water.
The article to be coated is merely dipped into the
solution.
POLISHERS.-Floor Polish.
Permanganate of potash in boiling water, applied to
the floor hot, will produce a stain, the color being
dependent on the number of coats. The floor may
them be polished with beeswax and turpentine.
For Furniture. Make a paste of
equal parts of plaster of paris, whiting, pumice
stone and litharge, mixed with Japan dryer, boiled
linseed oil and turpentine. This may be colored
to suit. This will fill the cracks of the wood.
Afterwards rub over the entire surface of the wood
with a mixture of 1 part Japan, 2 of linseed oil,
and three parts of turpentine, also colored, and after
this has been allowed to slightly harden, rub it off,
and within a day or two it will have hardened sufficiently
so that the surface can be polished.
Stove Polish. Ceresine, 12 parts;
Japan wax, 10 parts; turpentine oil, 100 parts; lampblack,
12 parts; graphite, 10 parts. Melt the ceresine
and wax together, and cool off partly, and then add
and stir in the graphite and lampblack which were
previously mixed up with the turpentine.
PUTTY.-Black Putty.
Whiting and antimony sulphide, and soluble glass.
This can be polished finely after hardening.
Common Putty. Whiting and linseed
oil mixed up to form a dough.
RUST PREVENTIVE.-For Machinery.
Dissolve an ounce of camphor in one pound of melted
lard. Mix with this enough fine black lead to
give it an iron color. After it has been on for
a day, rub off with a cloth.
For tools, yellow vaseline is the best substance.
For zinc, clean the plate by immersing
in water that has a small amount of sulphuric acid
in it. Then wash clean and coat with asphalt varnish.
SOLDERS.-For aluminum.
Use 5 parts of tin and 1 part of aluminum as the alloy,
and solder with the iron or a blow pipe.
Yellow hard solder. Brass, 3-1/2 parts; and zinc,
1 part.
For easily fusing, make an alloy of equal parts of
brass and zinc.
For a white hard solder use brass,
12 parts; zinc, 1 part; and tin, 2 parts.
SOLDERING FLUXES.-For soft
soldering, use a solution of chloride of zinc and
sal ammoniac. Powdered rosin is also used.
For hard soldering, borax is used most frequently.
A mixture of equal parts of cryolite
and barium chloride is very good in soldering bronze
or aluminum alloys.
Other hard solders are alloyed as
follows: brass, 4 parts; and zinc, 5 parts.
Also brass, 7 parts; and zinc, 2 parts.
Steel Tempering-.-Heat the steel red
hot and then plunge it into sealing wax.
For tempering small steel springs,
they may be plunged into a fish oil which has a small
amount of rosin and tallow.
VARNISHES.-Black Varnish.
Shellac, 5 parts; borax, 2 parts; glycerine, 2 parts;
aniline black, 6 parts; water, 45 parts. Dissolve
the shellac in hot water and add the other ingredients
at a temperature of 200 degrees.
A good can varnish is made by dissolving
15 parts of shellac, and adding thereto 2 parts of
Venice turpentine, 8 parts of sandarac, and 75 parts
of spirits.
A varnish for tin and other small
metal boxes is made of 75 parts alcohol, which dissolves
15 parts of shellac, and 3 parts of turpentine.
SEALING WAX.-For modeling
purposes. White wax, 20 parts; turpentine, 5
parts; sesame oil, 2 parts; vermilion, 2 parts.
Ordinary Sealin pounds of shellac,
1 pound Venice turpentine, add 3 pounds of vermilion.
Unite by heat.